ST52-3, also written St52-3, St 52-3 and DIN 17100 St52-3, is the legacy grade listed under material number 1.0570. St52-3N and ST52-3N make the normalized delivery condition explicit; they are not a different chemistry grade. S355J2, also written S355 J2 and EN 10025-2 S355J2, is a current quality in the EN 10025-2 S355 strength class, with steel number 1.0577.
ST52-3 and S355J2 sit in the same 355 MPa yield class at thickness up to 16 mm and share a −20 °C Charpy verification temperature, but they come from different standards, use different steel numbers, and are not automatic replacements for each other. The comparison below uses DIN 17100:1980-01 for DIN 17100 ST52-3 and EN 10025-2:2019 for EN 10025-2 S355J2.
ST52-3 vs S355J2 at a Glance
| Item | DIN 17100 ST52-3 (1.0570) | EN 10025-2 S355J2 (1.0577) |
|---|---|---|
| Standard status | DIN 17100:1980-01, withdrawn | EN 10025-2:2019, current |
| Steel number | 1.0570 | 1.0577 |
| Yield, 3–16 mm | 355 MPa min | 355 MPa min |
| Tensile strength, 3–100 mm | 490–630 MPa | 470–630 MPa |
| P and S, heat analysis | 0.040% max each | 0.025% max each |
| Impact, usual verification | N condition: −20 °C, 27 J (10–63 mm); 23 J (>63–100 mm) | −20 °C, 27 J longitudinal, ≤150 mm |
| Usual / permitted plate delivery | N usual for ST52-3 plate | +AR or +N at the manufacturer’s option unless the condition is ordered; +N must be stated if required |
Historical EN 10025-2 S355J2G3 carried material number 1.0570, but S355J2G3 is not a grade name in EN 10025-2:2019. The nearest current designation usually reviewed for normalized ST52-3 plate is EN 10025-2 S355J2+N, which keeps the S355J2 quality and states the +N delivery condition.
ST52-3 vs S355J2: Yield and Tensile by Thickness
| Nominal thickness | ST52-3 ReH min, MPa | S355J2 ReH min, MPa |
|---|---|---|
| 3–16 mm | 355 | 355 |
| >16–40 mm | 345 | 345 |
| >40–63 mm | 335 | 335 |
| >63–80 mm | 325 | 325 |
| >80–100 mm | 315 | 315 |
S355J2 yield values are from EN 10025-2:2019, Table 6, for flat products of width ≥600 mm, and they are the same for the other S355 qualities. They do not increase when +N is selected. The practical tensile difference at 3–100 mm is the 20 MPa lower minimum for S355J2 (470 MPa versus 490 MPa). Above 100 mm, DIN 17100 requires agreement, while EN 10025-2 continues tabulated values; those thicker EN bands are not a silent extension of a ST52-3 order.
Frequently Asked Questions (FAQ)
Is ST52-3 the same as S355J2?
No. They share a 355 MPa yield class at ≤16 mm and a −20 °C impact temperature, but ST52-3 is 1.0570 under withdrawn DIN 17100, while EN 10025-2 S355J2 is 1.0577 under current EN 10025-2, with a lower tensile minimum and tighter phosphorus and sulfur limits.
Should a ST52-3 order be filled with S355J2 as-rolled plate?
Not automatically. ST52-3 plate is usually supplied in the N condition. EN 10025-2 S355J2 may be delivered +AR unless +N is ordered. If the project needs normalized plate, state EN 10025-2 S355J2+N or another agreed +N designation.
Is S355J2G3 the current name for ST52-3?
EN 10025-2 S355J2G3 was the EN 10025:1993 designation that still carried 1.0570. It is not a grade name in EN 10025-2:2019 and is not identical to current S355J2 (1.0577).
For plate to DIN 17100 ST52-3 (1.0570) or EN 10025-2 S355J2, Please contact Gangsteel with the designation, edition, delivery condition, dimensions, quantity and any supplementary requirements. Learn more about our carbon and high-strength steel plate at Gangsteel.