EN 10025-6 quenched and tempered structural grades are sometimes compared with ASTM designations, but EN 10025-6 does not publish ASTM names as official equivalents. The official Gangsteel product pages list European and withdrawn-European designations, plus approximate Chinese GB/T 16270 strength-class names, and they treat those names as reference only, not as substitutes. This page records those official-page comparisons and, where an ASTM pointer exists, the one partial ASTM remark already published on EN 10025-6 S690Q.

EN 10025-6 Official-Page Equivalents (500 MPa class)

Item EN 10025-6 S500Q (1.8924) EN 10025-6 S500QL (1.8909)
ReH min, 3–50 mm 500 MPa 500 MPa
Rm, 3–50 mm 590–770 MPa 590–770 MPa
Impact, longitudinal minimum 30 J at −20 °C 30 J at −40 °C
P / S heat maxima, % 0.025 / 0.015 0.020 / 0.010

EN 10025-6 S500QL1 (1.8984) keeps the same strength table and is impact tested at −60 °C. Official remarks also cite withdrawn EN 10137-2 for the same grade names and steel numbers, and they cite GB/T 16270 Q500D or Q500E only as approximate strength-class names with different limits. No ASTM designation is published as a direct equivalent on the official EN 10025-6 S500Q or EN 10025-6 S500QL pages.

Where an ASTM Comparison Is Published

Item EN 10025-6 S690Q (1.8931) EN 10025-6 S500Q (for contrast)
ReH min, 3–50 mm 690 MPa 500 MPa
Rm, 3–50 mm 770–940 MPa 590–770 MPa
Official ASTM remark A514 / A517, partial only: similar yield class, different chemistry, impact and thickness rules No ASTM line is published on the official S500Q page
Property EN 10025-6 S500Q ASTM A572 Grade 50 (strength-class cross-reference only)
Minimum yield 500 MPa (3–50 mm) 50 ksi (345 MPa)
Tensile strength 590–770 MPa (3–50 mm) 65 ksi (450 MPa) min, ASTM A572/A572M Grade 50 specified tensile
Delivery / toughness basis Quenched and tempered; Charpy at −20 °C Different ASTM structural specification; not a quenched-and-tempered EN equivalent

A572 Grade 50 is tabulated only to show that a commonly named ASTM structural grade is a different, lower strength class. It is not an EN 10025-6 equivalent. Do not treat any ASTM grade as a replacement for an EN 10025-6 order unless the design documents accept that substitution.

Frequently Asked Questions (FAQ)

Is there a direct ASTM equivalent for EN 10025-6 S500Q?

Not on the official EN 10025-6 S500Q product page. That page lists EN 10025-6, withdrawn EN 10137-2 and an approximate GB/T 16270 name, and it does not publish an ASTM designation as a direct equivalent.

Which EN 10025-6 grade is compared with ASTM A514 or A517?

The official EN 10025-6 S690Q page cites A514 / A517 as a partial comparison only, at the 690 MPa yield class, and it states that chemistry, impact and thickness rules differ. That remark is not transferred here to the 500 MPa grades.

Can ASTM A572 Grade 50 replace an EN 10025-6 grade?

No. ASTM A572 Grade 50 has a 50 ksi (345 MPa) yield minimum, well below the 500 MPa class, and a different specification basis.

For plate to EN 10025-6, including S500Q or S690Q, Please contact Gangsteel with the designation, edition, delivery condition, dimensions, quantity and any supplementary requirements. Learn more about our carbon and high-strength steel plate at Gangsteel.

EN 10025-6 Equivalent ASTM Grades
Tagged on: