ASTM A516 Grade 60, also commonly written as A516GR.60, A516 Gr.60, A516 GR 60 and ASTM A516/A516M Grade 60 [Grade 415], is the inch-pound Grade 60 designation in ASTM A516/A516M. Grade 415 is the SI designation in the same specification, not a converted Grade 60 value. ASME SA516 Grade 60 (SA-516 or SA-516M Grade 60 or Grade 415) is the corresponding ASME family designation, not merely another spelling of the ASTM name. An ASTM-only certificate does not automatically satisfy a specified SA-516 order, and the reverse is also true. The official product page is ASTM A516 Grade 60.
ASTM A516/A516M does not itself contain an allowable-stress table. For ASME Section VIII, Division 1 (and other Sections that use Table 1A), the maximum allowable stress of SA-516 Grade 60 plate is taken from ASME BPVC Section II, Part D, Table 1A, for the designated product form, thickness, metal temperature and Code edition. The reference values below are public compilations of that table, for orientation only. Design calculations must use the Table 1A values and notes of the edition that governs the equipment.
Reference Allowable Stresses for SA-516 Grade 60 Plate (Table 1A)
Inch-pound and SI values are taken from independent compilations of Table 1A and are not exact conversions of one another. The customary series below is a published compilation of maximum allowable stress S for SA-516 Grade 60 plate, cross-checked at lower temperatures against other Table 1A extracts (17.1 ksi / 118 MPa) and, at higher temperatures, against a permitted metric reprint of Table 1A. The metric series is from that reprint (CIS GmbH page dated 2019, with ASME permission; CIS later describes its Table 1A tool as the 2021 Edition).
| Metal temperature, °F, not exceeding | Maximum allowable stress S, ksi (reference compilation) |
|---|---|
| −20 to 100, 150, 200, 250, 300, 400 and 500 | 17.1 |
| 600 | 16.4 |
| 650 | 15.8 |
| 700 | 15.3 |
| 750 | 13.0 |
| 800 | 10.8 |
| 850 | 8.7 |
| 900 | 5.9 |
| 950 | 4.0 |
| 1000 | 2.5 |
| Metal temperature, °C, not exceeding | Maximum allowable stress S, MPa (Table 1A metric reprint) |
|---|---|
| −30 to 40, through 250 | 118 |
| 300 | 115 |
| 325 | 112 |
| 350 | 108 |
| 375 | 104 |
| 400 | 88.9 |
| 425 | 75.3 |
| 450 | 62.7 |
| 475 | 45.5 |
| 500 | 31.6 |
| 525 | 21.9 |
| 550 | 12.7 |
Intermediate temperatures may be interpolated using the rounding rule in the Table 1A general notes of the governing edition. These figures are not a certified copy of the current ASME edition, and they do not replace the notes that accompany the official table.
Edition Notes and Temperature Limits That Travel with the Table
| Item | Reference statement (confirm in the governing edition) |
|---|---|
| Table 1A identification used here | SA-516 Grade 60 plate, UNS K02100, P-No. 1, Group 1, external-pressure chart CS-2, notes including G10, S1 and T2 in the compilations consulted |
| Section VIII, Division 1 maximum temperature listed | 1000 °F (538 °C) |
| Section I maximum temperature listed | 850 °F (454 °C) |
| Section III, Classes 2 and 3, maximum listed | 700 °F (371 °C) |
| Section XII maximum listed | 650 °F (343 °C) |
| Note G10 (graphite) | Upon prolonged exposure above 425 °C (about 800 °F), the carbide phase of carbon steel may be converted to graphite |
| Note T2 (time-dependent stresses) | In the metric reprint, stresses at 400 °C and above are obtained from time-dependent properties |
The 60–80 ksi (415–550 MPa) tensile range and the 32 ksi minimum yield disclosed on ASTM A516 Grade 60 are material test requirements. They are not allowable stress. An ASTM-only name is not automatically the Code designation used to read Table 1A; ASME design typically identifies the plate as SA-516 Grade 60 or SA-516M Grade 415.
Frequently Asked Questions (FAQ)
What is the allowable stress of ASTM A516 Grade 60?
ASTM A516 does not itself specify allowable stress. For ASME Section VIII, Division 1 work, the reference Table 1A value for SA-516 Grade 60 plate is 17.1 ksi (118 MPa) from −20 °F (−30 °C) through mid-range temperatures, then decreases at higher temperature as shown above. Use the Table 1A line and notes of the governing Code edition for design.
Can the 60–80 ksi tensile range be used as the allowable stress of ASTM A516 Grade 60?
No. 60–80 ksi is the public-reference tensile strength range for ASTM A516 Grade 60, not an allowable stress.
Why might a later ASME edition differ from the ASTM A516 Grade 60 values on this page?
Table 1A is revised by edition, and the official notes can change the usable value. The figures above are a reference compilation, not a substitute for the current Code tables.
Should an ASME allowable-stress table be read as ASTM A516 Grade 60 or as SA-516?
ASME Code design typically uses the SA-516 Grade 60 designation and the Table 1A line of the governing edition. An ASTM-only certificate does not automatically satisfy a specified SA-516 Code order.
For plate to ASTM A516/A516M Grade 60 [Grade 415] or ASME SA-516 Grade 60, please contact Gangsteel with the designation, edition, unit system, delivery condition, dimensions, quantity and any supplementary requirements. Learn more about our pressure-vessel and boiler steel plate at Gangsteel.