EN 10025-6 S690QL, also written S690 QL, EN10025-6 S690QL and steel number 1.8928, is a quenched and tempered structural plate with the same 690 MPa yield class as EN 10025-6 S690Q and a guaranteed Charpy test at −40 °C. The plate properties below are those already disclosed on EN 10025-6 S690QL.
These thickness rows follow the EN 10025-6:2004+A1 edition used on the official product page. The 2019 edition revised the thickness steps for thicker plates, so state the edition on the order and confirm the guaranteed value for the actual thickness on the mill certificate.
EN 10025-6 S690QL Plate Properties at a Glance
| Item | Published reference value / condition |
|---|---|
| Standard and quality | EN 10025-6, QL (Charpy at −40 °C) |
| Steel number | 1.8928 |
| Delivery condition | Quenched and tempered plate |
| ReH min, 3–50 / >50–100 / >100–150 mm | 690 / 650 / 630 MPa |
| Rm, 3–50 / >50–100 / >100–150 mm | 770–940 / 760–930 / 710–900 MPa |
| Elongation A min | 14% |
| Impact, longitudinal KV min | 50 J at 0 °C; 40 J at −20 °C; 30 J at −40 °C |
| Carbon, heat analysis max | 0.20% |
| P / S, heat analysis max | 0.020% / 0.010% |
EN 10025-6 S690QL Mechanical Properties
| Thickness (mm), 2004+A1 steps used on the official page | Yield strength ReH min (MPa) | Tensile strength Rm (MPa) | Elongation A min (%) |
|---|---|---|---|
| 3–50 | 690 | 770–940 | 14 |
| >50–100 | 650 | 760–930 | 14 |
| >100–150 | 630 | 710–900 | 14 |
Heat-analysis maxima on EN 10025-6 S690QL also include Si 0.80%, Mn 1.70%, N 0.015%, B 0.005%, Cr 1.50%, Cu 0.50%, Mo 0.70%, Nb 0.06%, Ni 2.0%, Ti 0.05%, V 0.12% and Zr 0.15%. Official CEV wording is that EN 10025-6:2019 maxima rise from 0.65 for plates up to 50 mm to 0.83 for the thickest plates. EN 10025-6 S690QL1 keeps the same strength table and is tested at −60 °C.
Frequently Asked Questions (FAQ)
What are the main plate properties of EN 10025-6 S690QL?
On EN 10025-6 S690QL, the thin-plate yield is 690 MPa, the tensile range is 770–940 MPa, elongation is 14% minimum, and longitudinal impact energy is 30 J minimum at −40 °C. Yield falls in the official thicker bands.
Does EN 10025-6 S690QL have the same plate strength as EN 10025-6 S690Q?
Yes, the official yield and tensile tables are the same. EN 10025-6 S690Q differs in the −20 °C impact quality and in higher phosphorus and sulfur maxima.
Do EN 10025-6 S690QL plate properties stay constant with thickness?
No. The official minimum yield is 690 MPa at 3–50 mm, 650 MPa above 50–100 mm and 630 MPa above 100–150 mm in the 2004+A1 steps used on the official page.
For plate to EN 10025-6 S690QL (1.8928), Please contact Gangsteel with the designation, edition, delivery condition, dimensions, quantity and any supplementary requirements. Learn more about our carbon and high-strength steel plate at Gangsteel.