ASTM A516 Grade 65, also commonly written as A516GR.65, A516 Gr.65, A516 GR 65 and ASTM A516/A516M Grade 65 [Grade 450], is the inch-pound Grade 65 designation in ASTM A516/A516M. Grade 450 is the SI designation in the same specification, not a converted Grade 65 value. ASME SA516 Grade 65 (SA-516 or SA-516M Grade 65 or Grade 450) is the corresponding ASME family designation, not merely another spelling of the ASTM name. An ASTM-only certificate does not automatically satisfy a specified SA-516 order, and the reverse is also true. The official product page is ASTM A516 Grade 65.
Hydrogen-induced cracking (HIC) testing is not a default requirement of the ASTM A516 Grade 65 designation. When sour-service resistance must be demonstrated, the usual method named on the order is NACE TM0284 (or the equivalent ISO document), together with the test solution, year, specimen plan and acceptance path. A “HIC-resistant” catalogue description, a tighter sulphur practice or the Grade 65 name is not, by itself, a recorded HIC result.
Common TM0284 Order Requirements
NACE TM0284 evaluates resistance to hydrogen-induced cracking by immersing specimens, typically for 96 hours at about 25 °C, in Solution A (acidified 5% sodium chloride / 0.5% acetic acid, pH about 3) or Solution B (artificial seawater, pH about 5), then sectioning them and reporting crack length ratio (CLR), crack thickness ratio (CTR) and crack sensitivity ratio (CSR). The ordering customer specifies which solution, how the ratios are averaged (per section, per specimen or per sample) and the acceptance limits.
When a purchase order invokes TM0284 Solution A and the example acceptance criteria of NACE MR0175 / ISO 15156-2 Table B.3, the figures commonly specified are as follows. They are common order values, not automatic A516 requirements, and many purchaser specifications use tighter limits.
| Item | Common order value | Condition |
|---|---|---|
| Test method and duration | NACE TM0284, 96 h, ambient temperature as required by the named edition | The document year must be written on the order |
| Test solution, if not otherwise specified | Solution A is the more severe, commonly specified solution | Solution B may be named instead when the specification does so |
| CLR (crack length ratio), Solution A | ≤ 15% | ISO 15156-2 Table B.3 example acceptance, commonly copied into purchase specifications |
| CTR (crack thickness ratio), Solution A | ≤ 5% | Same Table B.3 example value |
| CSR (crack sensitivity ratio), Solution A | ≤ 2% | Same Table B.3 example value |
| Tighter purchaser limits | Often 10/3/1, 5/3/1, or “zero cracking,” when the project specification says so | These are contract limits, not Table B.3 defaults and not A516 defaults |
The mill certificate should then show the actual method, solution, edition and results, not only the grade name. Chemistry limits for Grade 65, including the phosphorus and sulfur maxima discussed on ASTM A516 Grade 65, remain the composition requirements of the ordered edition. A purchaser may add tighter chemistry, vacuum degassing, a sulphur cap or a HIC test; those additions are contract requirements.
Other Sour-Service Documents Are Also Not Automatic
NACE MR0175 / ISO 15156 also contains material-selection limits that are sometimes written for carbon steel in sour service (for example restrictions on sulphur, phosphorus, nickel, hardness and strength). Those limits apply only when the project specifies that document. They are not automatically satisfied by ordering ASTM A516 Grade 65, and they do not replace a named HIC test when the order requires one.
| Item to state on a Grade 65 enquiry that needs HIC testing | Why it matters |
|---|---|
| Designation, edition and unit system | ASTM A516 or ASME SA-516 Grade 65 [Grade 450], as required, remains the plate specification |
| HIC document, year, solution and acceptance path | For example TM0284 (year), Solution A, and CLR/CTR/CSR limits, including how the ratios are averaged |
| Any tighter chemistry or other supplementary tests | These are additional contract items, not hidden parts of the Grade 65 name |
Frequently Asked Questions (FAQ)
Is HIC testing automatic for ASTM A516 Grade 65?
No. HIC or other sour-service requirements are supplementary. They apply to ASTM A516 Grade 65 only when the purchase order names them.
What HIC acceptance limits are commonly written for ASTM A516 Grade 65?
When NACE TM0284 Solution A and ISO 15156-2 Table B.3 are invoked, the commonly specified limits are CLR ≤ 15%, CTR ≤ 5% and CSR ≤ 2%. Many projects specify tighter numbers. None of these values is an automatic ASTM A516 Grade 65 requirement.
Does a “HIC-resistant” description prove ASTM A516 Grade 65 has been HIC tested?
No. A descriptive label is not a test result. Acceptance of ASTM A516 Grade 65 against a HIC requirement depends on the named method and the recorded results.
Does NACE MR0175 or ISO 15156 apply automatically to ASTM A516 Grade 65?
No. Those documents apply only when the project specifies them. The ASTM A516 Grade 65 designation does not, by itself, establish that compliance.
For plate to ASTM A516/A516M Grade 65 [Grade 450] or ASME SA-516 Grade 65, please contact Gangsteel with the designation, edition, unit system, delivery condition, dimensions, quantity and any supplementary requirements. Learn more about our pressure-vessel and boiler steel plate at Gangsteel.