St52-3, also commonly written as ST52-3, St 52-3 and DIN 17100 St52-3, is the legacy DIN 17100 St52-3 grade with material number 1.0570 (also written DIN 1.0570). St52-3N and ST52-3N make the normalized delivery condition explicit. These are written forms of the same DIN grade, not names of other standards.
The chemical composition of St52-3 is specified as heat-analysis maxima in DIN 17100:1980-01, Table 1. DIN 17100 is withdrawn. The limits below are the legacy quality-standard values for plate, not a current EN 10025-2 certificate and not typical mill results.
St52-3 Chemical Composition (Heat Analysis, Maximum %)
| Element / thickness basis | Heat analysis, mass % |
|---|---|
| C, thickness ≤30 mm | 0.20 max |
| C, thickness >30–100 mm | 0.22 max |
| C, thickness >100 mm | By agreement |
| Si | 0.55 max |
| Mn | 1.60 max |
| P | 0.040 max |
| S | 0.040 max |
| N | No numerical limit in the table (dash); nitrogen-binding elements required |
| Deoxidation | Special-killed, coded RR |
These are DIN 17100:1980-01, Table 1 ladle (heat) analysis maxima, not typical analyses and not product-analysis limits. A dash in the nitrogen column is not a zero-nitrogen requirement. Special-purpose KSt52-3 and RoSt52-3 variants have separate carbon footnotes and are not covered here.
What Each Limit Means for St52-3 Plate
| Requirement | Practical meaning |
|---|---|
| Thickness-dependent carbon | Plate over 30 mm may have up to 0.22% C; above 100 mm the limit must be agreed on the order |
| Mn up to 1.60% | Manganese provides most of the strength of this carbon-manganese structural steel |
| P and S up to 0.040% each | Higher than the 0.025% limits of current EN 10025-2 S355J2 |
| Special-killed (RR) with nitrogen-binding elements | Quality group 3 steelmaking; the N column has no numerical maximum |
| Same table for ST52-3N | The N suffix identifies normalized delivery and does not change the chemistry |
St52-3 vs Current S355J2 Chemical Limits
| Element | DIN 17100 St52-3 (1.0570) | EN 10025-2 S355J2 (1.0577) |
|---|---|---|
| C, ≤30 mm | 0.20% | 0.20% |
| C, thicker plate | 0.22% (>30–100 mm) | 0.22% (>30–400 mm) |
| Si / Mn | 0.55% / 1.60% | 0.55% / 1.60% |
| P / S | 0.040% / 0.040% | 0.025% / 0.025% |
| Cu, Ni, Cr, Mo | Not listed in the DIN plate entry used here | 0.55 / 0.42 / 0.29 / 0.11% max |
S355J2 values are from EN 10025-2:2019, Table 1. The comparison shows chemistry only. It is not a substitution approval: tensile range, delivery condition and edition must also be compared. For a new order, EN 10025-2 S355J2+N is the nearest current grade commonly reviewed.
Frequently Asked Questions (FAQ)
What is the chemical composition of DIN 17100 St52-3?
DIN 17100 St52-3 has heat-analysis maxima of C 0.20% up to 30 mm and 0.22% above 30–100 mm, Si 0.55%, Mn 1.60%, and P and S 0.040% each, from the 1980 edition, Table 1.
Does DIN 17100 St52-3 have a nitrogen limit?
Table 1 shows a dash in the nitrogen column for DIN 17100 St52-3 and requires additional nitrogen-binding elements. The dash is not a zero-nitrogen requirement and no numerical limit is borrowed from another grade here.
Is the chemistry of DIN 17100 St52-3N different from St52-3?
No. DIN 17100 St52-3N uses the same Table 1 chemistry. N identifies the normalized delivery condition only.
Is DIN 17100 St52-3 chemistry the same as S355J2?
Carbon, silicon and manganese maxima match, but S355J2 limits phosphorus and sulfur to 0.025% each, against 0.040% for DIN 17100 St52-3, and lists residual-element limits. The grades are not automatically interchangeable.
For plate to DIN 17100 St52-3 / ST52-3N, please contact Gangsteel with the standard edition, grade, delivery condition, dimensions and quantity. Learn more about our structural and high-strength steel plate at Gangsteel.