EN 10025-6 S550QL 1.8926 welding of high strength steel

Gangsteel supply EN10025-6 s550ql and EN10027-1 s550ql and EN10027-2 1.8926 steel plate. thickness 3mm to 180mm.Heat treatment of S550QL steel plate: Quenching and tempering (Q+T) S550QL is a European standard special alloy structural steel, attributed to quenched and tempered high yield strength structural steel, S indicates structural steel, 550 is the yield value, unit MPa, Q indicates delivery
Conditions, L indicates that the temperature is not lower than -50, the specified smaller value of impact energy, S550QL steel is a trademark in the EN 10025-6 specification, this specification rules that the smaller nominal thickness of the steel is 3mm, and the larger nominal thickness ≤
150mm.

EN 10027-1 S550QL 1.8926 high strength steel plate
EN 10027-1 S550QL 1.8926 high strength steel chart
EN 10027-1 S550QL 1.8926 high strength steel sheet
EN 10027-1 S550QL 1.8926 high strength steel for sale
EN 10027-1 S550QL 1.8926 high strength low alloy steel plate
EN 10027-1 S550QL 1.8926 high strength steel sheet metal
EN 10027-1 S550QL 1.8926 high strength carbon steel plate
EN 10027-1 S550QL 1.8926 plate slenderness limits for high strength steel sections
EN 10027-1 S550QL 1.8926 what is high strength steel plate
EN 10027-1 S550QL 1.8926 a high strength steel plate
EN 10027-1 S550QL 1.8926 high tensile strength steel plate
EN 10027-1 S550QL 1.8926 high tensile strength steel plates
EN 10027-1 S550QL 1.8926 high strength stainless steel plate
EN 10027-1 S550QL 1.8926 high strength steel plate australia
EN 10027-1 S550QL 1.8926 high strength weldable steel plate
EN 10027-1 S550QL 1.8926 ultra high strength steel plate
EN 10027-1 S550QL 1.8926 high yield strength steel plate
EN 10027-1 S550QL 1.8926 high strength alloy steel plate
EN 10027-1 S550QL 1.8926 high strength steel plate canada

News, Sports, Jobs.

Posted: Sun, 29 Nov 2020 07:15:19 GMT [source]

differential heating, n–heating that intentionally produces a temperature gradient within a steel object such that, after cooling, a desired stress distribution or variation in properties is current inside the object. direct quenching, n–in thermochemical processing, quenching instantly following the thermochemical therapy.

  • core, n–in clad products, the central portion of a multilayer composite metallic material.
  • core, n–in case hardening, the interior portion of unaltered composition or microstructure, or each, of a case hardened metal object.
  • important cooling price, n–the slowest fee of continuous cooling at which austenite can be cooled from above the transformation range to forestall its transformation above M s.

local steel supplier EN10025-6 S550Q 1.8924 steel plate

DISCUSSION–Unlike burning, it might be potential to revive the unique properties/microstructure by further warmth treatment or mechanical working, or a mixture thereof. grain progress, n–a rise in the grain size of a steel object, often as a result of exposure to elevated temperatures. graphitization annealing, n–annealing a metal object in such a method that some or the entire carbon is precipitated as graphite. hardenability, n–the property that determines the depth and distribution of hardness induced by quenching a steel object. hardening, n–rising the hardness by suitable remedy, normally involving heating and cooling.

 

What is different in EN10025-6 S550Q S550QL and S550QL1?

S550Q, S550QL, S550QL1 are European standard quenched and tempered high-strength structural steel plates.
S550Q, S550QL, S550QL1 organize production and implement European standard EN10025-6.
S550Q, S550QL, and S550QL1 conform to EN10029 standard for appearance quality deviation.
The main difference between S500, QS550QL and S550QL1 is low temperature impact toughness: Q means -20℃ impact; QL means -40℃ impact; QL1 means -50℃.

What is EN10025-6 S550QL Carbon Equivalent: CEV?

Thickness, mm

Max CEV based on the ladle analysis

5≤t≤50

0.65%

50<t≤100

0.77%

100<t≤150

0.83%

What is EN 10025-6 QT steel plate referring standard?
EN 1011-2 Welding-Recommendations for welding of metallic materials-Part 2: Recommendations for arc welding of ferritic steels
EN 10020: 2000 definition and classification of steel grades
EN 10025-1: 2004 Hot-rolled structural steel products-Part 1: General technical delivery conditions
EN 10027-1 Steel naming system-Part 1: Steel names and symbols
EN 10027-2 Steel naming system-Part 2: Steel number
EN 10163-1 Delivery requirements for surface conditions of hot-rolled steel plates, wide flat products and sections-Part 1: General requirements.
EN 10163-2 Delivery requirements for surface conditions of hot-rolled steel plates, wide flat products and sections-Part 2: Plates and wide flat products
EN 10164 Steel products with through-thickness performance-Technical delivery conditions

 

EN10025-6 S550QL Mechanical Properties

Grade

Thickness

Yield Strength

Tensile Strength

Elongation

Charpy V Notch Impact Test

Degree

Min Value

S550QL

mm

Min Mpa

Mpa

Min %

-40℃

J

5≤t≤50

550

640-820

16%

30

50<t≤100

530

640-820

30

100<t≤150

490

590-770

30

Note: Impact energy for impact test is on longitudinal

EN10025-6 S550QL Chemical Composition

Grade

The Element Max (%)

C

Si

Mn

P

S

N

B

S550QL

0.22

0.86

1.80

0.025

0.012

0.016

0.006

Cr

Cu

Mo

Nb

Ni

Ti

V

1.60

0.55

0.74

0.07

2.1

0.07

0.14

 

It also has close liaisons with European trade and professional organizations. The principal task of CEN is to prepare and problem European standards , outlined as a set of technical specs established and accredited in collaboration with the parties concerned in the various member international locations of CEN. They are established on the precept of consensus and adopted by the votes of weighted majority. Adopted standards must be applied in their entirety as national requirements by every member nation, regardless of the means by which the nationwide member voted, and any conflicting national requirements must be withdrawn. The identification of European requirements in every member country begins with the reference letters of the country’s national requirements physique, for example, BS for BSI in the United Kingdom, DIN for DIN in Germany, NF for AFNOR in France, etc. It is adopted by the initials EN and a sequential variety of as much as five digits. For instance, BS EN 10025, DIN EN 10025, or NF EN are all the identical EN normal, which can be found in English, French, and German.

This a part of EN offers the properties and other supply conditions for flat products for general functions, i.e. not for stress vessels nor for aerospace or other specialised functions, corresponding to springs, It is used for ordering functions. ASTM A283 plate metal options low and intermediate tensile energy carbon metal plate of structural high quality.

RG2 ULTRA HIGH STRENGTH STEELS Conventional direct hardening steels are normally designed ranges of tensile energy, which. four.3 For a new UNS quantity to be assigned, the composition have to be significantly different from that of any metal or alloy which has already been assigned a UNS quantity. four.three.1 In the case of metals or alloys that are usually recognized or specified by chemical composition, the chemical composition limits should be reported. 4.3.2 In the case of metals or alloys that are normally identified or specified by mechanical properties, such properties and limits thereof must be reported. Only those chemical components and limits, if any, that are vital in defining such supplies want be reported. four.4 Requests for brand new numbers shall be submitted on “Application for UNS Number Assignment” forms (see Fig. 1 and Fig. 2). Copies of those are available from any UNS numberassigning office or facsimiles could also be made of the one herein. ASTM International takes no place respecting the validity of any patent rights asserted in connection with any merchandise mentioned on this standard.

The same argument might be made when evaluating GS-33 CrNiMo and G30NiCrMo8 in the second group, where the differing nickel contents could be a foundation for rejection on a stricter comparison. A classic closest match instance is proven in Table 1.three, where compared to the three other steels on this group, the four grades inside EN are completely different; and some might argue that, on this basis, it does not belong to this comparative group. However, the Cr-Al-Mo alloys in this group are usually used as nitriding steels, and the EN steels are the closest match for this group. So excluding them would be a disservice to the user, since they belong to the identical software family and its inclusion on this group will direct the user to different similar nitriding alloys.

www alabama steel com EN10025-6 S550Q 1.8924 steel plate

manufacturers steel EN10025-6 S550Q 1.8924 steel plate

S355J2WP steel is a hot rolled structural metal with anti-corrosion function, also referred to as weathering metal and atmosphere corrosion resistance metal, beneath standard EN . 16Mo3 Steel is a EN10028 specified stress vessel grade chrome molybdenum steel alloy is used as a weldable metal within the fabrication of commercial boilers and steel pressurised vessels discovered in the oil. Description of Numbers Established for Metals and Alloys 2.1 The unified numbering system establishes 18 sequence of numbers for metals and alloys, as shown in Table 1. In most circumstances the letter is suggestive of the household of metals recognized; for instance, A for aluminum, P for valuable metals, and S for stainless steels.

used steel EN10025-6 S550Q 1.8924 steel plate

most steel EN10025-6 S550Q 1.8924 steel plate

For alloy steels, the first two digits of the SAE system describe the major alloying components present in the materials, the primary digit giving the alloy group. For example the 43XX series steels contain 1.65­2.00 % Ni, 0.50­0.80 % Cr and 0.20­0.30 % Mo, along with composition ranges for manganese and silicon and maximums for sulfur and phosphorus. Additional letters added between the second and third digits include “B” when boron is added (between 0.0005 and 0.003 %) for enhanced hardenability, and “L” when lead is added (between 0.15 and 0.35 %) for enhanced machinability. The prefix “M” is used to designate merchant quality steel (the least restrictive quality descriptor for decent-rolled metal bars utilized in noncritical elements of structures and equipment). The prefix “E” (electric-furnace metal) and the suffix “H” are primarily applicable to alloy steels. killed steel, n–a metal deoxidized to such a level that essentially no reaction occurred between carbon and oxygen throughout solidification. laser beam welding, n–a welding course of that makes use of a laser beam as the warmth source.

Contact Us
HENAN GANG IRON AND STEEL CO.,LTD
Email: admin@gangsteel.com

Phone: whatsapp: 0086-13598879167

Gangsteel produce EN10025-6 s550ql and EN10027-1 s550ql and EN10027-2 1.8926 steel plate. thickness 3mm to 180mm.Heat treatment of S550QL steel plate
, ,

Cold Rolled metal has an improved surface finish and tighter tolerances compared to sizzling rolled metallic. It is normally used for elements requiring chilly forming, similar to crimping, swaging or bending. It may also be used for Shafts, tools components, bolts, pinions, gears, in addition to within the creation of furniture, residence tools and different shopper items.

core, n–in clad merchandise, the central portion of a multilayer composite metallic material. critical cooling rate, n–the slowest fee of steady cooling at which austenite could be cooled from above the transformation range to prevent its transformation above M s.

Gangsteel trade item:
1.Payment Item: T/T,L/C
2.Trade Terms:CIF,FOB,CFR,CNF
3.Delivery Time: 10-30days
4. Steel Services: Cutting, Painting, shot blasting, Pretreatment, and The Third Party Inspection in DNV,BV, LR, GL, ABS, CCS , CE Mark, TUV, ISO, and others in super thick steel plate.
5.Packaging Details: Standard export seaworthy packing or as required.
6.Loading Port:Shanghai ,Tianjin, Qingdao.
7.Offer Ability:5000MT/Per Month.
8.MOQ:1 Pcs.

used steel EN10025-6 S550Q 1.8924 steel plate
Tagged on: